Note: Speeds are limited to 1500 RPM and lower for safety
Turning speeds are optimized for carbide tooling with a feed rate of (0.004/rev.), a depth of cut of 0.040, and a tool life of 180 minutes.
Material | AISI/SAE/ASTM Designation | Surface Feet/Minute |
Free machining plain carbon steels (resulfurized) | 1212, 1213, 1215 | 820 - 1045 |
Free machining plain carbon steels | 1108, 1109, 1115, 1117, 1118, 1120, 1126, 1211 | 950 |
Free machining plain carbon steels | 1132, 1137, 1139, 1140, 1144, 1146, 1151 | 670 - 800 |
Free machining plain carbon steels (Leaded) | 11L17, 11L18, 12L13, 12L14 | 800 - 820 |
Plain carbon steels | 1006, 1008, 1009, 1010, 1012, 1015, 1016, 1017, 1018, 1019, 1020, 1021, 1022, 1023, 1024, 1025, 1026, 1513, 1514 | 800 - 885 |
Plain carbon steels | 1027, 1030, 1033, 1035, 1036, 1037, 1038, 1039, 1040, 1041, 1042, 1043, 1045, 1046, 1048, 1049, 1050, 1052, 1524, 1526, 1527, 1541 | 670 - 970 |
Free machining alloy steels (resulfurized): | 4140, 4150 | 430 - 685 |
Water hardening tool steel | W1, W2, W5 | 590 |
Cold work, oil hardening tool steel | O1, O2, O6, O7 | 590 |
Cold work, air hardening tool steel | A2, A3, A4, A6, A7, A8, A9, A10 | 355 - 365 |
Stainless steels (Austenitic) | 201, 202, 301, 302, 304, 304L, 305, 308, 321, 347, 348 | 570 |
Cast Iron | ASTM Class 20, 25, 30, 35, 40 | 410 |
Brass | C35600, C37700, C36000, C33200, C34200, C35300, C48500, C34000 | 1170 |
Bronze | C65500, C22600, C65100, C67500 | 715 |
Wrought aluminum | 6061-T6, 5000, 6000, and 7000 series. | 2820 |
Cast aluminum | Sand and permanent mold casting alloys | 2820 |
Milling speeds are optimized for high speed steel tooling.
Material | AISI/SAE/ASTM Designation | Surface Feet/Minute |
Free machining plain carbon steels (resulfurized) | 1212, 1213, 1215 | 130 - 140 |
Free machining plain carbon steels | 1108, 1109, 1115, 1117, 1118, 1120, 1126, 1211 | 115 - 130 |
Free machining plain carbon steels | 1132, 1137, 1139, 1140, 1144, 1146, 1151 | 35 - 70 |
Free machining plain carbon steels (Leaded) | 11L17, 11L18, 12L13, 12L14 | 110 - 140 |
Plain carbon steels | 1006, 1008, 1009, 1010, 1012, 1015, 1016, 1017, 1018, 1019, 1020, 1021, 1022, 1023, 1024, 1025, 1026, 1513, 1514 | 65 - 110 |
Plain carbon steels | 1027, 1030, 1033, 1035, 1036, 1037, 1038, 1039, 1040, 1041, 1042, 1043, 1045, 1046, 1048, 1049, 1050, 1052, 1524, 1526, 1527, 1541 | 25 - 100 |
Free machining alloy steels (resulfurized) | 4140, 4150 | 35 - 100 |
Water hardening tool steel | W1, W2, W5 | 85 |
Cold work, oil hardening tool steel | O1, O2, O6, O7 | 50 |
Cold work, air hardening tool steel | A2, A3, A4, A6, A7, A8, A9, A10 | 40 - 50 |
Stainless steels (Austenitic) | 201, 202, 301, 302, 304, 304L, 305, 308, 321, 347, 348 | 70 - 75 |
Cast Iron | ASTM Class 20, 25, 30, 35, 40 | 70 - 100 |
Brass | C33200, C34000, C34200, C35300, C35600, C36000, C37700, C48500 | 100 - 200 |
Bronze | C22600, C65100, C65500, C67500 | 30 - 80 |
Wrought aluminum | 6061-T6, 5000, 6000, and 7000 series. | 165 |
Cast aluminum | Sand and permanent mold casting alloys | 165 |
Drilling and reaming speeds are optimized for high speed steel tooling.
Material | AISI/SAE/ASTM Designation | Drilling Surface Feet/Minute | Reaming Surface Feet/Minute |
Free machining plain carbon steels (resulfurized) | 1212, 1213, 1215 | 120 - 125 | 80 |
Free machining plain carbon steels | 1108, 1109, 1115, 1117, 1118, 1120, 1126, 1211 | 100 - 120 | 75 - 80 |
Free machining plain carbon steels | 1132, 1137, 1139, 1140, 1144, 1146, 1151 | 35 - 70 | 20 - 45 |
Free machining plain carbon steels (Leaded) | 11L17, 11L18, 12L13, 12L14 | 90 - 130 | 60 - 85 |
Plain carbon steels | 1006, 1008, 1009, 1010, 1012, 1015, 1016, 1017, 1018, 1019, 1020, 1021, 1022, 1023, 1024, 1025, 1026, 1513, 1514 | 60 - 100 | 40 - 65 |
Plain carbon steels | 1027, 1030, 1033, 1035, 1036, 1037, 1038, 1039, 1040, 1041, 1042, 1043, 1045, 1046, 1048, 1049, 1050, 1052, 1524, 1526, 1527, 1541 | 25 - 90 | 15 - 60 |
Free machining alloy steels (resulfurized) | 4140, 4150 | 30 - 90 | 15 - 60 |
Water hardening tool steel | W1, W2, W5 | 85 | 55 |
Cold work, oil hardening tool steel | O1, O2, O6, O7 | 45 | 30 |
Cold work, air hardening tool steel | A2, A3, A4, A6, A7, A8, A9, A10 | 30 - 50 | 20 - 35 |
Stainless steels (Austenitic) | 201, 202, 301, 302, 304, 304L, 305, 308, 321, 347, 348 | 50 - 55 | 30 - 35 |
Cast Iron | ASTM Class 20, 25, 30, 35, 40 | 80 - 100 | 50 - 65 |
Brass | C35600, C37700, C36000, C33200, C34200, C35300, C48500, C34000 | 160 - 175 | 160 - 175 |
Bronze | C65500, C22600, C65100, C67500 | 120 - 140 | 110 - 120 |
Wrought aluminum | 6061-T6, 5000, 6000, and 7000 series. | 350 - 400 | 350 - 400 |
Cast aluminum | Sand and permanent mold casting alloys | 350 - 400 | 350 - 400 |
Keywords | rpm calculator speed cutter turning drilling milling machining Suggest keywords | Doc ID | 82670 |
---|---|---|---|
Owner | Eric E. | Group | ECB Shops Documentation |
Created | 2018-06-05 15:10:13 | Updated | 2023-06-01 13:54:19 |
Sites | ECB Shops Documentation | ||
Feedback | 30 3 Comment Suggest a new document |